Our lengthy experience on the national market and the extent of our export business, qualify us as valid partners for every type of project. Considering this, we summarise hereunder our main productions, grouping them by prevalent deployment, with emphasis however on the fact that our plants regularly produce different alloys to client specification or according to standards and specifications from various Countries.
Our experienced technicians are at your disposal for any required service, in-depth analyses or study of new alloy or processing that may arise from the market or with clients.
Alloy designation | Cu | Pb | Al | Si | Fe | Sn max | Ni max | Mn max | As | Zn |
---|---|---|---|---|---|---|---|---|---|---|
Delta C (CB754S) | 58 – 62 | 0,5 – 2,4 | 0,10 – 0,80 | 0,05 max | 0,7 max | 1 | 1 | 0,5 | – | resto |
Lega Rubinetteria (CB753S) | 58 – 60 | 1,8 – 2,5 | 0,4 – 0,8 | 0,05 max | 0,5 – 0,8 | 0,8 | 0,5 – 1,2 | 0,20 | – | resto |
CB753S Ni 0,3% max (D.M. 174) | 59,0 – 60,0 | 1,8 – 2,5 | 0,4 – 0,8 | 0,05 max | 0,5 – 0,8 | 0,8 | 0,3 | 0,20 | – | resto |
Superpress | 60 – 61 | 1,7 – 2,3 | 0,2 – 0,4 | 0,15 – 0,35 | 0,5 max | 0,8 | 0,5 | 0,1 | – | resto |
OT 63 | 62,5 – 64,0 | 1,7 max | 0,3 – 0,5 | 0,6 – 0,9 | 0,6 max | 0,7 | 0,5 | 0,1 | – | resto |
OT 65 | 64,3 – 66 | 1,7 max | 0,3 – 0,5 | 0,6 – 0,9 | 0,6 max | 0,7 | 0,5 | 0,1 | – | resto |
Commercial designation | Density Kg/dm³ | Electrical conductivity % IACS | Machinability rating % (free-machining brass = 100) | Linear shrinkage % | Optimum casting range °C | Lower melting point °C |
---|---|---|---|---|---|---|
Delta C (CB754S) | 8,45 | 21 | 80 | 1,9 – 2 | 980 – 1080 | 885 |
Lega Rubinetteria (CB753S) | 8,45 | 21 | 80 | 1,9 – 2 | 980 – 1080 | 890 |
CB753S Ni 0,3% max (D.M. 174) | 8,45 | 21 | 80 | 1,9 – 2 | 980 – 1080 | 890 |
Superpress | 8,5 | 19 | 70 | 1,6 – 1,7 | 1040 – 1100 | 890 |
OT 63 | 8,37 | 15 | 85 | 1,8 – 1,9 | 1020 – 1100 | 900 |
OT 65 | 8,37 | 15 | 85 | 1,8 – 1,9 | 1020 – 1100 | 900 |
Commercial designation | Tensile strenght R N/mm² | Yield strenght Rr (0,2) N/mm² | Elongation A % | Hardness Brinell HB |
---|---|---|---|---|
Delta C (CB754S) | 390 – 440 | 150 – 200 | 22 – 25 | 90 – 110 |
Lega Rubinetteria (CB753S) | 390 – 440 | 150 – 200 | 23 – 28 | 90 – 110 |
CB753S Ni 0,3% max (D.M. 174) | 390 – 440 | 150 – 200 | 23 – 28 | 90 – 110 |
Superpress | 370 – 400 | 150 – 170 | 23 – 28 | 85 – 90 |
OT 63 | 370 – 430 | 150 – 190 | 25 – 35 | 90 – 105 |
OT 65 | 380 – 430 | 180 – 230 | 16 – 22 | 95 – 105 |